Process analysis of piston rod components

1. The piston rod is subjected to alternating loads during normal use, φ 50mm × There is a sealing device at 770mm that rubs its surface back and forth, so it requires high hardness and wear resistance.
Made of 38CrMoALA material, φ 50mm × After quenching and tempering treatment and surface nitriding, the 770mm part has a core hardness of 28-32HRC, a surface nitriding layer depth of 0.2-0.3mm, and a surface hardness of 62-65HRC. This gives it both toughness and good wear resistance.
2. The structure is relatively simple, but with a large aspect ratio, it belongs to the slender shaft type component and has poor rigidity. In order to ensure machining accuracy, rough and fine turning should be separated during turning, and both rough and fine turning should use a tool holder to reduce the deformation of the workpiece during processing. When processing threads at both ends, a holder should be used.
3. When selecting the positioning reference, in order to ensure the coaxiality tolerance of the components and the mutual position accuracy of each part, all processing processes adopt two central hole positioning, in accordance with the principle of unified reference.
4. When grinding the outer circular surface, the workpiece is prone to deformation of the tool and elasticity, which affects the accuracy of the piston rod. Therefore, during processing, the hole should be polished and kept clean, with appropriate tightness between the hole and the top and good lubrication. General selection of grinding wheel: abrasive white alumina (WA), particle size 60 #, hardness medium soft or medium to ceramic bonding agent. In addition, the width of the grinding wheel should be narrow to reduce radial grinding force. During processing, attention should be paid to the selection of grinding amount and the grinding depth should be small.
5. During grinding φ 50mm × When the outer circle is 770mm and the taper is 1:20, the two processes need to be carried out separately. When grinding a 1:20 taper, the test piece must be ground first, and only after passing the inspection can the workpiece be officially ground. 1: The inspection of the 20 cone surface is carried out using a standard 1:20 ring gauge for color coating, and the contact surface should not be less than 80%.
6. In order to ensure the stability of the machining accuracy of the piston rod, manual straightening is not allowed throughout the entire machining process.
7. During nitriding treatment, threaded parts, etc., should be protected with protective devices.

嗯嗯啊啊无遮挡国产在线观看| 五月精品在线区| 97超碰中文熟女| 夜夜 做爱精品| 欧美午夜一区二区福利视频| 亚洲中文字幕无码在线| 播放中国美女日逼| 无码激情欧美| 国产精品女人久久久| 欧美日韩av在线| 嗯嗯啊啊嗯嗯嗯啊啊啊视频网站| 亚洲AV一二| 97精产国品一二三产区区别| WWW,亚洲少妇AV,Com| 影音先锋AV在线资源| 性色av 成人在线| 365久久爱| 男人的天堂.com| 国产AVove| 欧美精品稀缺资源在线观看| 超碰在线性| 伊人伊人鲁| av草逼美女| av天七猫精品| 一本加勒比天天日| 亚洲成a人片在线观看中文| 熟妇俱乐部视频| 欧美熟妇视频婷婷久久| 无码成人AV| 亚洲精品成人视频网站在线| 亚洲av无码精品色午夜| 涩涩涩涩在线| Av无码人妻| 欧洲美女一区精品视频| 成人av在线精品资源| 日韩欧美专区| 国产精品第一页第二页第三页 | 男女性色日韩AV网| 久久精品国产99精品国产亚洲性色 | 无码人妻天天爽夜夜爽精品91| 美女高潮免费19|